Casting method of marine propeller made of large copper alloy material
Feb 15, 2023
What is the casting method of large copper alloy marine propeller? Let's introduce it to you.
Melting
Since the gross weight of the propeller is 57t, two 30t medium-frequency electric furnaces are used for smelting, and the proportion of ZCuAl9Fe4Ni4Mn2 material is strictly followed. The smelting temperature is controlled at 1200~1250 ℃. Chemical composition analysis and bending angle test are conducted in the furnace to determine whether the alloy liquid meets the requirements. When it is qualified, it can be discharged. Since two pouring ladle of different sizes are used for pouring at the same time, the temperature in each pouring ladle must be controlled. In order to ensure that the pouring temperature is controlled within the required range, the discharging time and temperature of each furnace must be arranged in advance.
Degassing and gas content detection
Because the copper alloy is easy to inhale, mainly hydrogen. In order to obtain high-quality castings, the ladle bottom nitrogen blowing process is adopted. The dried nitrogen is blown into the alloy liquid through the ladle bottom. During the rise of the nitrogen bubble, the hydrogen dissolved in the copper liquid is taken away, and the metal inclusions in the alloy liquid also float up, so as to achieve the purpose of degassing and purifying the alloy liquid.
For the gas content test of copper liquid, the air pressure is generally controlled above -0.092MPa, and the sample is deemed to be qualified if it is not convex. If the above requirements are not met, nitrogen blowing shall continue until qualified.
Pouring
Stop nitrogen blowing after the gas content is qualified. For ZCuAl9Fe4Ni4Mn2 alloy, when pouring large castings, the pouring temperature can be between 1120 and 1140 ℃. Generally, the lower line temperature is taken for pouring, which can meet the requirements. When pouring, the riser feeding shall be conducted at an interval of 40~60min, so as to ensure the sequential solidification of the casting, improve the riser feeding effect and improve the internal quality of the casting.
Combined with the casting process design of large propeller, the appropriate shrinkage, deformation, processing capacity and other process parameters are considered; Adopting multi-furnace smelting and controlling reasonable smelting temperature, degassing process and pouring temperature are the preconditions to ensure the smooth pouring of castings. Through the design of bottom pouring system and adding high temperature copper liquid to feed the riser after pouring to 1/3 of the riser to ensure the sequential solidification of the casting, this is the key factor to obtain the internal quality of the casting.